Correlating Substrate Surface Finish Dissolution Kinetics with Reflow Profile Thermal Mass Variations

Optimizing reflow profiles for thermal mass variations controls substrate surface finish dissolution kinetics, preventing intermetallic embrittlement and scrap.

08.11.26 17 min

Dissolution

Automated surface mount technology machinery operates within a dark industrial enclosure while an autonomous mobile robot waits on the factory floor.

Kinetics of Finish Stripping in Molten Solder

Liquid solder attacks metallic substrate finishes as soon as physical contact occurs at elevated reflow temperatures. Finish erosion follows Arrhenius kinetics, governed primarily by activation energy, local peak bath temperature, and total dwell time above liquidus. In tin-lead and lead-free alloys like SAC305 (96.5% Sn, 3.0% Ag, 0.5% Cu), liquid tin acts as a solvent for base substrate coatings.

Electroless Nickel Immersion Gold (ENIG), Immersion Silver (ImAg), Immersion Tin (ImSn), and Organic Solderability Preservatives (OSP) present fundamentally distinct dissolution behaviors under thermal stress. The gold layer on ENIG dissolves almost immediately into molten solder at typical processing temperatures of 235°C to 245°C, stripping away within two to three seconds and exposing the underlying nickel-phosphorus layer to liquid tin.

Liquid solder dissolves nickel much slower than copper or gold, allowing the nickel layer to function as a diffusion barrier that shields the underlying copper foil. When thermal mass variations across a printed circuit board force extended dwell times, however, this nickel layer continuously reacts with tin to form binary intermetallics. High phosphorus content within the electroless nickel deposit ~ typically 7% to 11% by weight ~ accumulates at the interface as nickel is selectively consumed by the solder alloy.

Excess consumption leaves behind a nickel-depleted, phosphorus-rich phase known as the black pad precursor phase, which turns brittle and susceptible to impact failure if thermal exposure exceeds maximum limits.

Copper pads with Immersion Silver or OSP dissolve directly into liquid solder, with copper entering liquid SAC305 at rates between 0.05 and 0.15 micrometers per second at 240°C. This dissolution enriches the local liquid solder matrix with copper solute. When local copper concentration exceeds the saturation limit of approximately 1.2% by weight at 240°C, hexagonal crystal precipitates of intermetallic compounds nucleate within the bulk solder joint upon cooling. These floating intermetallic structures increase solder matrix rigidity, elevate the effective liquidus temperature of the remaining alloy, and introduce micro-voiding near pad interface zones.

Dissolution Kinetics and Intermetallic Layer Formation Rates for PCB Surface Finishes in SAC305 Solder
Substrate Surface Finish Dissolution Rate at 240°C (µm/s) Primary Intermetallic Phase Critical Exposure Dwell Limit (s) Dominant Failure Mode Under Over-Exposure
Electroless Nickel Immersion Gold (ENIG) 0.01 to 0.03 (Ni layer) (Ni,Cu)3Sn4 / Ni3Sn4 120 Phosphorus-rich layer brittle fracture
Electroless Nickel ENEPIG 0.01 to 0.02 (Ni layer) (Pd,Ni)Sn4 / (Ni,Cu)3Sn4 150 Palladium embrittlement at joint margin
Immersion Silver (ImAg) 0.08 to 0.12 (Base Cu) Cu6Sn5 / Cu3Sn 90 Excessive base copper erosion and voiding
Immersion Tin (ImSn) 0.05 to 0.10 (Base Cu) Cu6Sn5 / Cu3Sn 75 Pre-reflow intermetallic consumption
Organic Solderability Preservative (OSP) 0.06 to 0.14 (Base Cu) Cu6Sn5 / Cu3Sn 90 Pad cratering due to deep Cu diffusion
Operators inspect extruded elastomer profile gaskets inside an industrial manufacturing plant during final factory assembly operations.

Immersion Tin and Silver Erosion Thresholds

Immersion coatings rely on complete displacement during the early liquidus phase. Standard immersion tin deposits range from 0.8 to 1.2 micrometers in thickness. Storage thermal history and prior reflow cycles convert raw immersion tin into solid-state copper-tin intermetallics before final assembly reflow.

During the primary reflow pass, whatever unreacted tin remains dissolves within less than one second, leaving the solid-state intermetallic layer exposed to liquid solder. Extended time above liquidus allows liquid tin to penetrate through grain boundaries of this primary intermetallic phase, attacking the underlying copper substrate.

Immersion silver coatings present a different interfacial reaction mechanism. Silver dissolves rapidly into liquid solder within 0.5 seconds of contact, dispersing completely into the bulk alloy matrix and leaving the underlying copper pad unprotected. High thermal mass areas on a printed circuit board require prolonged heating to reach reflow temperature, extending the liquid phase duration for nearby low-mass components.

Low thermal mass pads coated with immersion silver undergo prolonged exposure to liquid solder, driving total copper dissolution depth beyond 2.5 micrometers and thinning traces beneath small surface-mount pads, which reduces mechanical fatigue resistance under operational thermal cycling.

SAC305 solder at 245°C dissolves surface copper at 0.11 micrometers per second, consuming 3.3 micrometers of pad thickness during a thirty-second liquidus extension.
Architectural material samples featuring textured panels and fabric swatches are displayed beside a minimalist ceramic vessel in a production studio.

Barrier Layer Consumption Dynamics

In ENEPIG finishes, a 0.05 to 0.15 micrometer palladium layer sits between the gold and nickel, retarding the initial dissolution rate of nickel into liquid solder. Palladium dissolves into liquid tin at approximately 0.2 micrometers per second at 240°C. Once this barrier enters the solder solution, the nickel layer undergoes controlled dissolution. Dissolved palladium within the interfacial solder matrix modifies the crystallization pathway during solid-state cooling, suppressing the formation of continuous brittle intermetallic plates.

However, excess heat input from surrounding high thermal mass structures can entirely deplete thin nickel deposits on fine-pitch pads, exposing bare copper beneath and causing catastrophic joint dewetting.

Solder joint strength varies with chemical plating bath conditions, though surface finish thickness variations within standard vendor tolerances generally remain within acceptable reflow assembly windows.

Mass

A heavy duty steel articulating bracket mounts a circular wooden platform to a dark grey wall inside an industrial design showroom.

Copper Weight Variations and Heat Absorption

Physical distribution of copper across individual circuit layers creates localized thermal gradients during reflow processing. Printed circuit boards combining mixed copper weights ~ such as inner signal layers with 0.5-ounce copper adjacent to heavy power planes with 3-ounce copper ~ exhibit non-uniform heat absorption profiles because high copper volume functions as a localized thermal sink. During infrared or convection reflow heating, zones containing solid copper planes require greater total thermal energy to achieve target peak temperatures than signal-dense zones containing minimal copper.

Component dimensions exacerbate these thermal mass differentials across the assembly surface. Large metal-shielded inductors, high-pin-count ball grid arrays (BGAs), and aluminum electrolytic capacitors absorb massive quantities of thermal energy during the ramp-to-peak phase. Small 0201 or 0402 ceramic chip capacitors situated adjacent to these heavy components experience severe thermal shadowing, delaying the rate at which neighboring solder joints reach melting temperature.

To ensure that solder joints beneath heavy BGAs achieve the minimum required liquidus temperature of 217°C for SAC305, operators elevate conveyor heat zone setpoints or slow down conveyor speeds.

Elevating furnace heat input causes low thermal mass regions to experience extreme thermal over-exposure. Solder joints located on isolated, low-mass pads remain above liquidus temperature for extended durations, sometimes reaching temperatures exceeding 255°C while heavy components barely achieve 225°C. The temperature delta across a single assembly can exceed 30°C in unoptimized reflow profiles. This wide delta creates divergent dissolution kinetics across the board surface: low thermal mass pads undergo aggressive finish dissolution and excessive intermetallic growth, while high thermal mass pads suffer from incomplete wetting, cold joints, or head-in-pillow defects.

Various material samples rest on a structured stone testing bench inside a manufacturing facility quality control laboratory.

Thermal Gradient Mapping across High-Density Boards

Engineers profile thermal density variations by placing thermocouples across diverse board locations during process setup to identify the minimum and maximum thermal nodes. The minimum thermal node corresponds to the heaviest component lead or center ground pad tied directly to an internal copper plane, whereas the maximum thermal node corresponds to an isolated, low-density signal pad near the outer board edge. Profiling reveals the differential heating rate between these locations during the soak and peak reflow phases.

Thermal mass differences directly govern local liquidus entry timing. Solder paste on low thermal mass pads melts up to fifteen seconds earlier than paste on adjacent high thermal mass nodes. Liquid solder on low-mass pads begins dissolving the surface finish while neighboring high-mass joints are still solid.

This extended liquid state on low-mass nodes accelerates chemical dissolution of the surface finish metal, depleting protective barrier layers before the cooling ramp begins.

Standard assembly specifications permit a maximum temperature delta of 10°C across all component nodes at the point of peak reflow temperature entry.

Uncorrected thermal gradients inevitably degrade assembly yields. Surface finishes must be evaluated not only for their as-received solderability, but for their structural endurance under extended thermal exposure. Process engineers mapping reflow windows must account for the specific failure modes triggered by localized thermal over-exposure across high-density layouts.

  • Head-in-Pillow Voiding occurs when high thermal mass leads delay solder paste coalescence, allowing pad finish dissolution to complete while the component lead remains out of thermal equilibrium.
  • Pad Cratering Instability results from extended thermal exposure over low-mass copper planes, inducing high inter-laminar stress and deep copper depletion beneath the pad surface.
  • Intermetallic Layer Embrittlement develops when low thermal mass pads spend excess time above liquidus temperature, driving nickel layer consumption past critical phosphorus-enrichment thresholds.
  • Trace Necking Failure arises on fine-pitch signal lines tied to low thermal mass pads where liquid solder dissolves base copper beyond twenty percent of original trace width.

Designing copper pour patterns with thermal relief geometries around surface-mount pads maintains consistent thermal mass across assembly nodes regardless of internal plane connections.

Profile

A modular architectural model featuring a gradient thermal channel and metallic plates rests upon a neutral grey tabletop next to a ceramic vessel.

Engineering Thermal Profiling for Mixed Density

Reflow profile construction balances two opposing thermal limits across the circuit assembly. The minimum profile envelope must supply sufficient heat energy to melt solder paste and completely dissolve surface finishes across high thermal mass nodes where heavy copper delays heating. The maximum profile envelope must restrict heat exposure across low thermal mass nodes to prevent thermal degradation of substrates and excessive finish dissolution kinetics.

Achieving this balance requires precise manipulation of preheat ramp rates, soak duration, zone temperature offsets, and conveyor speed.

Convection reflow ovens feature independent heating zones equipped with top and bottom heating elements. Multi-zone furnaces allow thermal engineers to shape the temperature-time trajectory. A prolonged thermal soak stage between 150°C and 180°C equalizes board temperatures prior to entering the peak reflow zone.

Extending soak duration reduces the temperature delta between high-mass and low-mass nodes to less than 8°C, though it also increases total thermal exposure, initiating solid-state diffusion between the surface finish and base copper before solder melting occurs.

  1. Install calibrated thermocouples at the highest thermal mass ground pad, the lowest thermal mass signal pad, and the center body of the highest mass component using high-temperature silver epoxy.
  2. Run a baseline profile pass through the convection furnace at a standard conveyor speed of 85 centimeters per minute with uniform zone temperature setpoints.
  3. Analyze thermocouple data to identify the temperature spread between the minimum thermal node and maximum thermal node at the moment the maximum node reaches 217°C.
  4. Adjust upper heating zone temperatures in the soak stage to increase heat transfer into high thermal mass zones while holding lower heating zone temperatures steady.
  5. Reduce conveyor speed incrementally until the highest thermal mass node maintains a minimum time-above-liquidus of 45 seconds at a peak temperature of at least 232°C.
  6. Verify that the lowest thermal mass node does not exceed a maximum time-above-liquidus of 90 seconds or a maximum peak temperature of 250°C during the optimized pass.

Conveyor speed directly governs dwell time across all thermal zones as thermal mass alters heating response. Slowing the conveyor increases total time-above-liquidus for every pad on the board. The profile optimization process must ensure that while high thermal mass nodes achieve proper wetting and voiding control, low thermal mass nodes remain within safe kinetic dissolution thresholds.

Time-Above-Liquidus and Peak Temperature Variations Across Assembly Nodes Under Unoptimized vs. Optimized Profiles
Profile Optimization State Node Location Thermal Mass Class Peak Temperature (°C) Time-Above-Liquidus (s) Dissolution Depth (µm)
Unoptimized Baseline Profile Isolated Signal Pad Low Thermal Mass 258 108 2.8 (Cu)
Unoptimized Baseline Profile BGA Center Ground Pad High Thermal Mass 219 38 0.4 (Cu)
Soak-Equalized Profile Isolated Signal Pad Low Thermal Mass 248 78 1.9 (Cu)
Soak-Equalized Profile BGA Center Ground Pad High Thermal Mass 228 52 0.9 (Cu)
Fully Optimized Zone-Offset Profile Isolated Signal Pad Low Thermal Mass 242 64 1.3 (Cu)
Fully Optimized Zone-Offset Profile BGA Center Ground Pad High Thermal Mass 234 58 1.1 (Cu)
Material finish samples and textured fabric swatches rest inside an industrial design binder on a dark workstation surface.

Zone Temperature Offsets and Conveyor Cadence

Modern reflow ovens permit differential temperature settings between top and bottom heating modules within the same longitudinal zone. Utilizing top-to-bottom zone offsets directs heat energy onto heavy component bodies while mitigating heat transfer into exposed bottom-side copper layers. Top-side heating modules in the peak reflow zone can be set 15°C higher than bottom-side modules.

This offset forces thermal energy into large component bodies from above, bringing heavy component leads to liquidus temperature rapidly without requiring elevated bottom-side convection that would overheat isolated low-mass signal traces.

A reflow profile that limits temperature differentials across thermal nodes to under ten degrees preserves surface finish integrity across all component pads.

Master supply agreements typically incorporate standard manufacturing tolerances for printed circuit board reflow processing. IPC-7095D states that thermal profiles for ball grid array assemblies must maintain solder joint peak temperatures between 235°C and 245°C across all ball locations. Specifying this range in assembly purchase orders binds the contract manufacturer to perform node-specific thermal mapping, preventing profile configurations that induce excessive finish dissolution on low thermal mass pads.

Microstructure

An industrial inspector examines metal surface finish swatches arranged on shelves inside a manufacturing quality assurance laboratory.

Intermetallic Compound Layer Evolution

Interfacial chemical reactions between liquid solder and metallic surface finishes dictate joint microstructural development. The reaction layer formed at the solder-substrate interface consists of intermetallic compounds whose composition取决于 the base surface finish metallurgy. On bare copper or OSP coatings, liquid tin reacts with copper to form a duplex intermetallic layer consisting of eta-phase (Cu6Sn5) adjacent to the solder matrix and epsilon-phase (Cu3Sn) adjacent to the copper substrate, with both phases growing continuously throughout reflow.

Extended time-above-liquidus driven by high thermal mass profile requirements alters intermetallic layer growth dynamics. Total intermetallic layer thickness increases as a function of the square root of time above liquidus. Under nominal reflow conditions (60 seconds above 217°C), the Cu6Sn5 layer forms a scalloped morphology between 1.0 and 1.5 micrometers thick.

When low thermal mass nodes endure extended liquidus times up to 120 seconds, the Cu6Sn5 layer grows beyond 3.0 micrometers into thick, continuous planar structures. Prolonged thermal exposure also accelerates solid-state diffusion of copper into the intermetallic boundary, thickening the brittle, planar Cu3Sn phase layer underneath.

Electroless nickel surfaces alter microstructural evolution by introducing a nickel barrier. Solder joints formed on ENIG surfaces exhibit a ternary intermetallic phase layer consisting of (Ni,Cu)6Sn5 or Ni3Sn4 depending on the copper concentration within the solder paste matrix. As liquid tin reacts with the nickel deposit, phosphorus is rejected from the forming intermetallic compound structure and accumulates at the interface as a thin, amorphous nickel-phosphorus layer (Ni3P).

Excessive thermal exposure drives high nickel dissolution, expanding the Ni3P layer thickness beyond 200 nanometers and predisposing the solder joint to brittle interface cleavage under mechanical shock or vibration.

Intermetallic Compound Phase Characteristics and Thickness Evolution Under Variable Reflow Thermal Mass Profiles
Substrate Finish Type TAL Duration (s) Peak Temperature (°C) Intermetallic Phases Formed Total IMC Thickness (µm) Interfacial Shear Strength (MPa)
ENIG 45 230 Ni3Sn4, Ni3P (thin) 0.8 48.5
ENIG 110 252 (Ni,Cu)6Sn5, Ni3P (thick), Ni2SnP 2.4 31.2
ENEPIG 50 232 (Pd,Ni)Sn4, (Ni,Cu)6Sn5 0.9 51.0
ENEPIG 115 250 (Ni,Cu)6Sn5, Ni3P 1.8 44.3
OSP (Copper) 40 228 Cu6Sn5 (scalloped) 1.2 42.1
OSP (Copper) 115 254 Cu6Sn5 (planar), Cu3Sn (continuous) 3.6 24.8
Various industrial material panels hang above a conference microphone positioned on a dark workbench inside a development facility.

Which Substrate Finishes Resist Extended Liquidus Times?

Selecting substrate finishes for circuit boards containing extreme thermal mass variations demands careful assessment of finish degradation thresholds. ENEPIG finishes demonstrate superior resistance to extended thermal dwell times compared to standard ENIG or OSP because the intermediate palladium layer buffers the nickel surface against immediate liquid tin attack, maintaining barrier integrity even when low thermal mass pads spend over 90 seconds above liquidus temperature. Immersion silver provides excellent surface coplanarity for fine-pitch components but suffers from rapid copper erosion when exposed to elevated temperatures, making it less suitable for heavy copper, mixed-density assemblies.

Evaluating finish suitability requires matching metallurgical stability with assembly profile constraints. Quality engineers must systematically select surface finishes based on measured thermal delta parameters across the target board layout rather than relying on nominal specs.

  • ENEPIG Finish Selection applies to assemblies with thermal deltas exceeding 20°C where low-mass nodes endure long liquidus times while high-mass nodes reach melting points.
  • Direct Immersion Gold Specification is restricted to single-density board geometries with uniform thermal mass distribution across all surface pads.
  • High-Phosphorus ENIG Selection mandates strict controls on maximum time-above-liquidus to prevent hyper-passive black pad formation on low thermal mass nodes.
  • OSP Finish Implementation requires dense copper plane thermal relief structures to eliminate localized copper erosion on fine-pitch signal traces.
Cross-sectional metallography confirms that interfacial intermetallic layer thickness exceeding four micrometers correlates with a fifty percent reduction in drop-shock survival rate.

Microstructural examination of failed solder joints often reveals micro-cracking running parallel to the substrate interface along the Cu3Sn or Ni3P phase boundary. Whether solid-state aging at elevated operating temperatures accelerates this brittle phase transformation faster in ENEPIG or high-phosphorus ENIG finishes under real-world thermal cycling remains subject to ongoing field degradation studies.

Ledger

A bent metallic strip displaying precision machining marks rests on a textured stone slab with translucent material in the background.

Commercial Cost of Thermal Profile Over-Exposure

Financial losses resulting from uncompensated thermal mass variations manifest through multiple operational channels. Direct scrap during primary assembly represents the immediate cost: solder joint voiding, head-in-pillow defects, and component damage caused by excessive reflow temperatures inflate scrap rates on complex assemblies. A high-density, multi-layer printed circuit board assembly containing expensive BGAs, processors, and specialized surface finishes can carry a raw material cost exceeding 450 USD per unit.

Scrapping ten units per production shift due to profile-induced solder failures generates a direct material loss of 4,500 USD per day.

Rework increases unit cost. Repairing defective solder joints under high-density components requires localized heat application using hot-gas rework stations, subjecting the targeted pad and surrounding components to an additional thermal cycle. This second thermal exposure drives further dissolution of the substrate surface finish and thickens the existing intermetallic layer.

Solder joints subjected to double reflow processing exhibit up to 35% lower fatigue resistance than primary joints. Field returns caused by latent intermetallic embrittlement cleavage incur massive warranty liabilities, recall expenses, and customer support costs that far outstrip initial assembly margins.

Quantifying the financial impact of surface finish degradation requires analyzing production yield against profiling optimization expenses. Dedicated thermal profiling hardware, multi-channel data loggers, and node-specific thermocouple installation add non-recurring engineering costs during production NPI setup, but these initial setup investments guard against chronic yield loss later.

  • Thermocouple Harness Assembly requires 150 USD per test board in materials and two technician hours for silver-epoxy mounting and calibration.
  • Reflow Optimization NPI Dwell consumes four hours of line machine time, valued at 600 USD per hour in lost throughput capacity.
  • Cross-Sectional Metallurgical Audit costs 350 USD per coupon evaluation to measure intermetallic thickness and barrier layer consumption profiles.
  • Field Failure Warranty Reserve accrues at 2.5% of total shipment value when processing unoptimized mixed thermal mass assemblies.
Industrial metal components and assorted surface finish swatches rest on a clean workbench inside a manufacturing facility with large windows.

Worked Financial Model for Scrap and Rework Yields

Consider a high-volume manufacturing run of 50,000 complex server motherboards featuring heavy copper internal planes and fine-pitch BGAs. Assume a baseline unoptimized reflow profile yields a first-pass scrap rate of 3.2% driven by head-in-pillow voids on high thermal mass nodes and pad cratering on low thermal mass nodes. At a manufacturing cost of 220 USD per unit, scrapping 3.2% of the run equates to 1,600 failed units, generating a direct financial loss of 352,000 USD.

Implementing an advanced profiling protocol with zone-offset heating and ENEPIG surface finish specification requires an upfront investment of 18,000 USD in NPI engineering, specialized profiling runs, and surface finish material premiums.

Optimizing the reflow process drops the first-pass defect rate to 0.4%, resulting in only 200 scrapped units valued at 44,000 USD. Net savings from process optimization equal 290,000 USD on a single production batch, paying back the upfront investment in thermal profile engineering and surface finish dissolution control within the first 3,500 manufactured units.

Contractual terms between OEM buyers and electronics manufacturing services (EMS) providers must define explicit liabilities for profile-induced microstructural defects. Standard supply contracts often assign scrap costs to the EMS provider only if defects exceed an agreed Acceptable Quality Level (AQL) threshold, typically set at 0.65% for Class 2 electronics under IPC-A-610 standards. If the contract fails to specify thermal mass gradient limits and surface finish dissolution criteria, the EMS provider may run aggressive, high-temperature reflow profiles to maximize line speed.

This operational shortcut achieves acceptable first-pass visual inspection rates while delivering microstructurally degraded joints to the buyer, transferring latent warranty failure risk entirely onto the OEM balance sheet.

Nomenclature

Dwell Time

Meaning ~ Administrative monitoring of cargo duration establishes the operational window during which containers occupy port facilities before departure or after arrival.

Surface Finish Erosion

Meaning ~ Gradual degradation of the protective metal coating on printed circuit board copper pads occurs when the board is exposed to harsh chemical environments or repeated heating cycles.

Printed Circuit Board

Meaning ~ Insulating substrate with conductive copper tracks used to mechanically support and electrically connect electronic components forms the physical foundation of almost all modern electronic assemblies.

Cu3Sn Phase

Meaning ~ A metallurgical intermetallic layer forms at the interface between copper substrates and tin-based solders during the heating cycles of electronic assembly.

Intermetallic Compound

Meaning ~ Crystalline substance forms between different metal elements during the soldering process and provides the essential metallurgical bond between the component and the circuit board.

Intermetallic Layer

Meaning ~ Microscopic zones of intermediate phases formed by chemical reactions between different metals during soldering or welding provide the essential metallurgical bond.

Microstructural Degradation

Meaning ~ Progressive breakdown of internal grain structures and lattice formations under environmental stress determines the loss of mechanical property values over a service interval.

Surface Finishes

Meaning ~ A manufacturing specification standard that defines the texture, coating, chemical passivation, and protective treatment applied to the exterior of a fabricated component.

Convection Reflow

Meaning ~ Thermal processing stages placed downstream from surface-mount component placement melt solder paste to form permanent metallurgical bonds across circuit assemblies.

Electroless Nickel

Meaning ~ Chemical deposition represents a method of applying a metal coating to a solid substrate without the application of an external electrical current.

Copper Weight Variation

Meaning ~ Fluctuation in the mass of copper cladding on printed circuit board layers affects the electrical impedance and thermal performance of the finished electronic assemblies.

Hot Gas Rework

Meaning ~ Localized application of heated gas to melt solder joints allows the safe extraction and replacement of defective components on populated circuit boards.

What the firm knows, published

Expertise is a utility, not a secret. sentiention™ publishes its working knowledge as open reference: intelligence layer covering the materials it sources, the markets it enters, and the reference that serves both.