Meaning
An intermetallic compound of copper and tin forms at the interface between copper pads and tin-based solder during the reflow soldering process. The presence of hexacoppertin pentastannide indicates a successful metallurgic bond between the solder and the substrate. This compound has a hexagonal or monoclinic crystal structure depending on the temperature.
It is essential for mechanical connection but can become a source of failure if it grows too thick.
Metallurgical Evolution
Reflow temperatures above the melting point of the solder accelerate the diffusion of copper into the molten tin. As diffusion occurs, hexacoppertin pentastannide quickly nucleates as scalloped grains along the copper pad. During subsequent solid-state aging, the compound continues to grow, albeit at a slower rate.
This continuous growth can consume the copper layer and lead to the formation of a secondary, copper-rich intermetallic phase called tricopper stannide.
Reliability Concern
Excessive thickness of the intermetallic layer introduces brittleness to the solder joint. Because hexacoppertin pentastannide is harder and more brittle than the bulk solder, the interface becomes sensitive to mechanical shock and thermal cycling. Stresses generated by differences in thermal expansion coefficients concentrate at the interface.
This structural vulnerability leads to brittle fracture under drop testing or vibration.
Process Mitigation
Controlling the peak temperature and time-above-liquidus during reflow restricts the initial growth of the intermetallic layer. Adding small amounts of nickel, cobalt, or other dopants to the solder paste helps to refine the grain structure of hexacoppertin pentastannide and slow down its growth during service. This microalloying approach stabilizes the solder joint by creating a more uniform interface.
In addition, using nickel-based surface finishes like electroless nickel immersion gold acts as a diffusion barrier to copper. This barrier effectively prevents the rapid growth of the intermetallic compound and enhances the long-term reliability of electronic assemblies in harsh operating environments.